Grades | Stainless Steels | SA-1008 SHS Grade 26[180]

AMS SA-1008 SHS Grade 26[180] ( Precipitation-Hardening )

PDF | Word | Print

SA-1008 SHS Grade 26[180] Application:Specification for Steel, Sheet, Cold-Rolled, Carbon, Structural, High-Strength Low-Alloy and High-Strength Low-Alloy With Improved Formability

Chemical composition(mass fraction)(wt.%) of the SA-1008 SHS Grade 26[180]
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.06
Si - 0.75
Mn - 0.75
P - -
S - -
Ni - 0.50
Cr 25.00 27.00
Al - -
Cu - 0.20
Ti - -
Fe - -
N - 0.04
Mo 0.75 1.50

Mechanical properties of grade SA-1008 SHS Grade 26[180]

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
476 (≥) 235 (≥) 31 43 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 213

Physical properties of grade SA-1008 SHS Grade 26[180]

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
435 (≥) 932 (≥) 13 11 41 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
642 639 262 - - -

SA-1008 SHS Grade 26[180] Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED